提出以“云边一体化架构”构建硅钢智慧决策系统,来解决原硅钢制造L1~L5系统架构模式下的数字信息孤岛、业务功能割裂等问题。在此基础上,开发了云边协同的自学习型控制模型及业务决策模型,构建起硅钢“智慧大脑”,形成了以研发、制造、服务等核心业务数字化融合的智能化决策支持新模式,探索出一条钢铁制造业数字化、智能化转型之路。 SIDS(Silicon-steel Intelligent Decision-making System)based on \"cloud-edge integration architecture\" was proposed to solve the problems of data silos and business function fragmentation in the original L1~L5 system architecture.On this basis,the self-learning control model and decision-making model of cloud-edge collaboration were developed,the \"smart brain\" of silicon steel department was constructed,and a new intelligent decision-making support model of digital integration of core businesses s... 
2022-02-28 243 5.8

本发明公开了一种高磁感取向硅钢,其含有Fe及不可避免的杂质元素,其还含有质量百分含量如下的下述各化学元素:C:0.02~0.08%,Si:2.0~4.5%,Mn:0.02~0.30%,S≤0.0050%,Als:0.01~0.04%,N:0.002~0.01%,Nb:0.0050~0.0600%;以及P:0.01~0.1%,Sn:0.01~0.30%,Cu:0.01~0.50%的至少其中一种。此外,本发明还公开了上述高磁感取向硅钢的制造方法,其包括步骤:(1)制得板坯;(2)板坯加热;(3)热轧,其包括:粗轧、在热卷箱内卷取保温,以及精轧;其中粗轧结束温度高于970℃;卷取温度为800~1050℃,卷取时间为30~200s;精轧开始温度低于1050℃;(4)冷轧;(5)脱碳退火;(6)渗氮;(7)涂覆退火隔离剂;(8)高温退火;(9)涂覆绝缘涂层和激光刻痕。
2021-10-19 224 6.8

本发明公开了一种硅钢环形炉内罩的内圆直径自动检测装置及方法,该内圆直径自动检测装置包括设置在检测点地面上的水平工作台,设置在所述水平工作台上的水平调节机构,设置在所述水平工作台上的扫描机构,以及与所述扫描机构通信互联的检测处理机构。该内圆直径自动检测装置是非接触式设备,不受内罩温度的限制,使用方便灵活,设备可靠性好,安全性高,对环境无污染,不仅能够有效节约校圆机的使用频次,而且大大增强了炉子的安全可靠性。
2021-03-25 180 6.8

一种适用于取向电工钢产线的一体化生产计划排程方法,基于L4,建立基于如下步骤的整条取向电工钢产线的自动生产计划排程,S1:以排程所需的必要数据为基础,按核心工序为排程起点,分别依次递进式完成前工序、后工序的排程,形成初始计划排程;S2:对初始计划排程建立基于设定的评价因子构成的综合评估,形成由综合评估结果构成的综合评估结果数据集;S3:对综合评估结果数据集建立优化算法运算,根据运算结果确定生产计划排程。本发明的一种适用于取向电工钢产线的一体化生产计划排程方法,可实现较大程度的自动化,提高生产计划编制效率,增强操作人员对生产计划的整体情况掌握,并可根据设备状态及计划执行情况自动对计划作出快速响应。
2021-08-25 234 6.8

本发明公开了一种用于无取向硅钢清洗液的洁净度检测分析方法,包括以下步骤:步骤1:从清洗液循环槽中取含有污物的清洗液样品,并进行脱水、烘干、研磨,得到污物粉末样品;步骤2:根据含有污物的清洗液样品和污物粉末样品计算清洗液循环槽中清洗液的洁净度;步骤3:根据含有污物的清洗液样品的洁净度建立清洗液洁净度评定标准;步骤4:根据清洗液洁净度评定标准控制含有污物的清洗液的排放和换液。本发明能简便且直观的了解当前清洗段循环槽内清洗液的状态,并可以根据清洗液的洁净度评级对清洗液的使用和排放做出及时的在线调整。
2021-06-21 239 6.8

本发明公开了一种利用取向硅钢氧化镁废弃物生产镁质球团的方法,采用取向硅钢生产过程中的废氧化镁污泥、废氧化镁粉等氧化镁废弃物,以及粗粒铁矿粉、镜像赤铁矿、磁铁精矿、膨润土和石灰石粉为原料,依次经预处理、配料、造球后,再在链箅机‑回转窑‑环冷机上进行干燥预热、焙烧和冷却,得到镁质球团。本发明利用氧化镁废弃物制备镁质球团,既有利于减少氧化镁废弃物带来的环保压力及其外运时产生的处置费用,也能显著降低镁质球团的制造成本,综合利用了钢铁厂的现有资源,生产出环境友好、低成本的镁质球团,为高炉提供优质原料,最终降低炼铁过程的污染物排放,减少环境污染。
2021-01-15 174 6.8

采用RH精炼添加钙合金方式对硅钢进行钙处理,结果表明,钙合金添加量为0.67、1.00和1.67 kg/t钢时,钢中Ca含量分别为0、2×10-6和4×10-(6质量分数);随着钙合金添加量的增加,钢中夹杂物粒度逐渐由0~2μm向2~4μm、4~6μm偏移;不同钙处理条件下,钢中均存在粒径小于1μm和粒径为1~5μm的MnS、CuxS夹杂物,后者或单独存在,或与AlN、CaS夹杂复合;钢中粒径为5~10μm的夹杂物基本以Ca的氧化物和硫化物为主。与未经钙处理的炉次相比,钙合金添加量为0.67、1.00和1.67 kg/t钢时,粒径小于1.0μm的夹杂物减少幅度分别为68.06%、87.50%和94.94%。钙合金添加量为1.67 kg/t钢时,可以去除钢中绝大部分的微细夹杂物。 In order to improve the properties of final silicon steels,the calcium treatment was adopted by adding Ca alloys into the liquid steel during the RH refining process.Results show that when the addition of Ca alloys is 0.67 kg/t,1.00 kg/t and 1.67 kg/t,the corresponding Ca content in silicon steels is 0,2 × 10-6 and 4 × 10-6 respectively.With the increase of Ca alloy addition,the particle sizes of inclusions in steels become 2~4 μm and 4~6 μm,from 0~2 μm.Under different calcium treatments,there e... 
2013-02-28 249 5.8

一种基于大数据分析技术的电工钢用户选材询单推荐方法,于终端计算机内、以可与终端计算机各数据库进行信息交互的形式、设置一计算模块;经此计算模块完成依次的基于各数据库的有效信息的采集、用户询单选材推荐方案模型的设置、基于有效信息及推荐方案模型完成推荐牌号的生成,根据设定的评估模型对生成的推荐牌号及信息评估运算的运行,据此建立对用户的选材询单推荐。本发明的一种基于大数据分析技术的电工钢用户选材询单推荐方法,基于L4计算机系统开发出的计算模块及相应的可与计算模块进行信息交互的用户界面完成,形成可根据不同用户需求对应的不同评价体系,完成与不同用户需求适配的方案推荐。
2021-07-23 249 6.8

采用RH精炼添加钙合金方式对硅钢进行钙处理。结果表明,钙合金添加量为0.67、1.00、1.67kg/t钢时,钢中钙含量分别为0、2×10-6、4×10-6;随着钙合金添加量增大,钢中夹杂物粒度逐渐由0~2μm向2~4、4~6μm偏移;不同钙处理条件下,钢中均存在粒径小于1μm和粒径为1~5μm的MnS、CuxS夹杂物,后者或单独存在,或同AlN、CaS夹杂复合;粒径为5~10μm区间,钢中的夹杂物基本以钙的氧、硫化物为主。与钙处理前相比,钙合金添加量为0.67、1.00、1.67kg/t钢时,粒径小于1.0μm的微细夹杂物减少幅度分别为68.06%、87.50%、94.94%。钙合金添加量为1.67kg/t钢时,可以去除钢中绝大部分的微细夹杂物。 Ca alloy was added into the liquid steel during RH refining,and the results show that Ca concentration in final Si steel sheets is insignificant,about 0,2×10-6 and 4×10-6 when the added amount of Ca is 0.67,1.00 and 1.67 kg/t steel,respectively.With the increase in the added Ca alloy amount,the inclusions in the steel gradually change from those of 0~2 μm to those of 2~4 and 4~6 μm.Under different Ca treatments,there exist MnS and CuxS inclusions whose size is below 1 μm as well as MnS and CuxS ... 
2013-02-28 345 5.8

某冷连轧机生产无取向硅钢板材时,其边缘降的长度合格率频繁超标。为满足用户的叠片厚度精度要求,这类产品必须以增大切边量的方式来保证交货质量,而这种方式又直接降低了金属收得率,提高了生产成本。基于此,以该产线现有设备特性为基础,详细分析其软、硬件功能模式,分别对辊形与反馈控制进行全面分析与优化改进。通过现场试验论证,充分明确依托辊形优化与反馈控制程序的改进能显著提高边缘降的控制水平,该技术的使用为生产现场的边缘降控制提供了合理的技术支撑。 A cold rolling mill production of non-oriented silicon steel sheet,the thickness difference of the edge( edge-drop) is usually exceed the preset standard value,In order to meet the accuracy requirements of the user flatness,these production must be trimed wider length to meet the delivery quality of the user need, which directly reduce the metal yield and increase the manufacturing cost. Therefor,the software and hardware of the production line has been analyzed, and the work roll shape and feed... 
2014-02-28 301 5.8

针对宝钢硅钢常化退火过程中产生的退火炉辊印缺陷问题,通过实际生产的大数据与产品质量问题相结合,将数据挖掘、数据分析方法应用到实际,一定程度上解决了现场实际生产中的痛点,为现场生产提供决策支撑,避免了以前通过人工识别判定存在疏漏和无法定量判断的问题,形成了一套具有鲁棒性和可操作性的钢铁生产过程数据分析方法。通过智慧决策系统平台获取实际生产和表检仪数据,基于Pearson相关系数算法进行变量挑选和特征工程,并应用随机森林算法对数据建立分类预测模型,实现了质量问题的溯源和监控,通过数据量化预测了炉辊印缺陷是否可通过轧制消除的质量问题,识别准确率达到96.43%。 In views of the normalizing annealing furnace roll marks problem occurred in the process of normalizing annealing of silicon steel in Baosteel,by combining big data from actual production with product quality problems,data mining and data analysis methods were applied to actual production to solve the pain points and provide decision support,a robust and practical data analysis method for the steel production process has been developed,which avoided the previous problems of omission and non-quan... 
2022-01-28 259 5.8

结合工业化生产的无取向硅钢,进行了RH精炼喂CaSi线去除钢中的非金属夹杂物试验研究。针对不同的钙处理条件,分析了CaS夹杂生成热力学,观察了夹杂物的形貌和尺寸分布,确定了夹杂物的类型、数量,探讨了钙处理后钢中夹杂物的变化规律。结果表明,本试验条件下,钙处理可以有效抑制MnS、AlN夹杂物的生成,有效促进钢中微细夹杂物的聚合、上浮、去除,钢质纯净度明显提高。经过合适的钙处理后,钢中的夹杂物以独立存在的CaO为主,同时有少量含CaO、SiO2、MgO的复合夹杂,没有发现CaS夹杂存在。这部分夹杂物的尺寸集中分布在2~20μm,数量约为1.8×105个/mm3。 Experimental study on removal of non-metallic inclusions in non-oriented silicon steel obtained from industrial production by CaSi wire feeding during RH refining process was carried out.The thermodynamics of CaS inclusion formation was analyzed,the morphology and the size distribution of inclusions were observed,and the numbers and types of inclusions were also determined for the steel specimens treated under different calcium treatment conditions.Furthermore,the variation of inclusion characte... 